R/t Limits for Bending and Stamping: Why Coated Steel Cracks at 1.0

Fabex Engineering Team October 24, 2026
R/t Limits for Bending and Stamping: Why Coated Steel Cracks at 1.0 — Sheet metal stamping

R/t Limits for Bending and Stamping: Why Coated Steel Cracks at 1.0

The inside radius divided by the material thickness (R/t) is the number that decides whether a bend survives — not the radius on its own, and not the material grade alone — and at R/t = 1.0 the outer surface of the sheet is stretched by roughly a third of its length in a single operation. Mild steel tolerates that. A 22 µm zinc-magnesium coating does not, which is why S250GD+ZM310 bent to one thickness cracks along the radius while the steel underneath is still intact, and why the part is rejected even though it did not break.

This is a working guide to the ratio, the limit for the materials we form most often, and the gap between the limit and the ideal — the value you should actually put on a drawing.

Why the ratio decides, not the radius

Bending does not crack metal by folding it; it cracks it by stretching the outside of the fold. For an inside radius R and thickness t, with the neutral axis taken at mid-thickness, the outer fibre is stretched by approximately:

ε_outer  ≈  t / (2R + t)   =   1 / (2·(R/t) + 1)

The consequence is that a 3 mm radius means nothing on its own. In 1 mm sheet it is R/t = 3, a comfortable bend. In 6 mm plate the same 3 mm radius is R/t = 0.5, and the outer fibre is stretched by half its length. Expressing the limit as a ratio removes the ambiguity, and it is why mill datasheets and drawing notes both work in multiples of thickness.

R/t Outer-surface strain What survives it
0.5 50% Almost nothing except very soft, fully annealed steel
1.0 33% Cold-rolled mild steel; most coatings fail here
1.5 25% Mild steel, 304 stainless, soft aluminium; thick coatings marginal
2.0 20% Most formable grades; standard coatings; prepainted borderline
2.5 17% High-strength steel, heavy coatings, prepainted
3.0 14% Dual-phase steel, work-hardened aluminium
4.0 11% Titanium, hardened tempers, 6061
8.0 6% Bends that are really just gentle curves

Two corrections matter in practice. The neutral axis does not sit exactly at mid-thickness: at tight radii the K-factor falls towards 0.35–0.42, which shifts the neutral axis towards the inside and raises the real outer-fibre strain — at R/t = 1.0 with K = 0.42 it is closer to 41% than 33%. And tensile elongation (A80) is not a substitute for the ratio: it measures uniform plus post-uniform extension over an 80 mm gauge, while a bend imposes a steep local gradient with much of the section well below the limit. Both effects mean the tables below are guidance for design, not a substitute for a formed coupon in the actual material.

Outer-fibre strain plotted against inside radius to thickness ratio: 33% at R/t 1.0, falling to 17% at R/t 2.5 and 6% at R/t 8

A bending limit is therefore two numbers: the limit, where the first crack appears, and the ideal, where the process is stable across coil-to-coil variation, tooling wear and operator skill. Designing to the limit means the tenth part cracks after the first article passed.

The substrate limit for the materials we stamp most

Indicative minimum and recommended R/t for a 90° bend at room temperature, bending across the rolling direction, in air bending or a drawn feature. Structural grades are shown with the yield-strength band they represent, because that band is what moves the number.

Material Typical grades Limit R/t Recommended R/t
Cold-rolled mild steel DC01, SPCC 0–0.5 1.0
Deep-drawing mild steel DC04, DC05, SPCE 0 0.5–1.0
Hot-rolled mild steel S235, S275, Q235 1.0 1.5
Structural steel S355 1.0–1.5 1.5–2.0
HSLA, moderate strength S315MC–S420MC 1.5–2.0 2.0–2.5
HSLA, high strength S500MC, S700MC 2.0–3.0 3.0–4.0
Dual-phase AHSS DP590, DP780 1.5–2.5 2.5–3.5
Dual-phase AHSS DP980 3.0–4.0 4.0–5.0
Austenitic stainless, annealed 304L, 316L 1.0–1.5 1.5–2.0
Ferritic stainless 430, 439 0.5–1.5 1.5–2.0
Strain-hardened stainless 301 half-hard 2.0–3.0 3.0–4.0
Aluminium, soft 1050, 3003-O 0.5–1.0 1.0–1.5
Aluminium, work-hardened 5052-H32, 5754-H22 1.5–2.0 2.0–2.5
Aluminium, heat-treated 6061-T6 4.0–6.0 6.0 or avoid the bend
Copper, annealed C110 0.5–1.0 1.0–1.5
Brass, half-hard C260 1.5–2.5 2.5–3.0
Titanium Grade 2 / Grade 5 2.0–3.0 / 4.0+ 3.0–4.0 / avoid at room temperature

The full table with the underlying justification sits in minimum bend radius by material, and the aluminium-specific caveats are in what is the minimum bend radius for aluminium. Three patterns explain almost all of it:

  • Strength and formability trade against each other. Moving from a 250 MPa structural grade to a 700 MPa one takes the radius from about 1.5t to about 3t, because the material that resists the load also resists the deformation.
  • Temper matters more than alloy. 5052 in the O condition forms at 1t; the same alloy at H34 needs 2–3t. 6061-T6 is not a formed component at all in most shops.
  • Work hardening accumulates. A second bend close to the first sees material that has already been stretched, so the effective limit for the second bend is one band stricter than the table.

What a coating adds — and why ZM310 is the marginal case

Everything above describes cracking the steel. A coated sheet has a second, thinner, much less ductile surface that must follow the same strain, and it usually fails first.

Hot-dip zinc is the most forgiving because zinc is comparatively ductile and the coating is a single phase. Zn-5%Al (Galfan) forms a fine eutectic and behaves almost as well. The two coatings that cause most of the trouble are the ones chosen for corrosion performance:

Zn-Al-Mg (ZM, of which Magnelis is the best-known example). The microstructure is a zinc-rich primary phase with a eutectic network containing hard MgZn₂ intermetallic — deliberately, because the magnesium is what gives the coating its cut-edge protection and its resistance to red rust. That intermetallic network is the first thing to crack. Once it does, the crack runs across the bend, and the coating’s whole reason for existing — a continuous barrier that protects sheared edges — starts at a discontinuity.

Zn-55%Al (AZ, Aluzinc). Aluminium-rich dendrites with an interdendritic zinc phase. Excellent corrosion resistance, harder and less ductile than zinc, and similarly prone to fine transverse cracking at tight radii.

The relevant thickness is small but not negligible. EN 10346 expresses coating mass as the total for both faces, so ZM310 is 155 g/m² per face, about 22 µm of coating on each side; Z275 is roughly 19 µm; AZ150 is roughly 19 µm on an aluminium-rich alloy. At R/t = 1.0 the coating surface must stretch by a third of its length alongside the steel, and 22 µm of intermetallic-containing metal simply cannot redistribute that strain the way the 0.8 mm substrate can.

For prepainted and coil-coated sheet the failing layer is the organic film. A polyester topcoat elongates by roughly 20–30% before it crazes; PVDF is lower; a thick plastisol is higher but is normally used on profiles that are roll-formed rather than press-bent. The coating’s adhesion is usually the real limit: the film can stretch, but the interface between primer and zinc cannot resist the shear that comes with it, so the failure appears as loss of adhesion and underfilm corrosion rather than an open crack.

Cross-section of a 22 micron Zn-Al-Mg coating cracking at R/t 1.0 and staying intact at R/t 2.5 on the same 0.8 mm steel

Coating-limited R/t: the numbers to design to

The coating limit replaces the substrate limit whenever it is stricter, which for a heavy zinc-magnesium or prepainted surface it usually is. Values are indicative for 90° bends across the grain at room temperature; the mill datasheet and the customer’s specification always take precedence.

Surface Typical coating per face Limit R/t Recommended R/t
Bare, oiled — substrate limit substrate + 0.5
Electrogalvanised, thin ZE25–ZE75, ≈2–5 µm 0.5–1.0 1.0–1.5
Hot-dip zinc, light Z100–Z140, ≈7–10 µm 0.5–1.0 1.5
Hot-dip zinc, heavy Z275, ≈19 µm 1.0 1.5–2.0
Zn-5%Al ZA255, ≈18 µm 1.0 1.5–2.0
Zn-55%Al AZ150, ≈19 µm 1.0–1.5 2.0
Zn-Al-Mg, light ZM60–ZM120 1.0–1.5 1.5–2.0
Zn-Al-Mg, medium ZM200 1.0–1.5 2.0
Zn-Al-Mg, heavy ZM310, ≈22 µm 1.5–2.0 2.0–2.5
Prepainted polyester film 20–25 µm, T-bend 2T 1.5–2.0 2.0–3.0
Prepainted PVDF or high-build film 25–30 µm, T-bend 2T–3T 2.0–2.5 3.0
Powder or wet paint after forming 60–100 µm substrate limit substrate + 0.5

A note on the coating column: for hot-dip products the per-face figure is the nominal half of the designation, but EN 10346 specifies a triple-spot minimum, so one face can be thinner than the arithmetic suggests. Where the coating mass matters to the bend, specify the minimum single-spot value rather than the nominal total.

The prepainted rows map to the T-bend test in EN 13523-7, which folds a strip through 180° with n sheet thicknesses between the legs. A rating of 2T means no cracking when bent back on itself with two thicknesses inserted, and corresponds roughly to an inside radius of 2t — a harsher test than a 90° production bend, which is why a product rated 2T is generally usable at R/t ≈ 1.5–2 on the press brake.

Bar chart of limit and ideal R/t ranges for bare mild steel, Z275, AZ150, ZM200, ZM310, prepainted polyester and S700MC sheet

Worked example: 0.8 mm S250GD+ZM310 at R/t = 1.0

This is the case that most often comes through a design review, and it is worth following the chain of consequences.

The drawing asks for a 0.8 mm inside radius. At t = 0.8 mm that is R/t = 1.0, and the outer fibre is strained by 33%, nearer 41% once the true neutral axis is considered. The steel is a 250 MPa structural grade and survives. The 22 µm Zn-Al-Mg coating does not: the MgZn₂ network cracks across the bend, the cracks are visible under a magnifier, and if the acceptance criterion is “no coating crack to substrate”, the part fails.

The fix is a radius, not a new material. Raising the inside radius to 1.6 mm (R/t = 2) drops the outer-fibre strain to 20%, and 2.0 mm (R/t = 2.5) drops it to 17%. Either passes; 2.0 mm leaves margin for the next coil.

The radius is set by the die, not by the drawing. In air bending the inside radius follows the die opening:

R  ≈  V / 6      (V = V-die opening)

So an inside radius of 2.0 mm needs a V-die of about 12 mm, whereas the die an operator would reach for by default — 6–8 mm for 0.8 mm sheet — produces a radius of 1.0–1.3 mm, which is exactly the condition that cracks the coating. This is the practical trap: the part is not made wrong, it is made with the standard tooling for the gauge.

Inside radius R/t at 0.8 mm Outer strain V-die (R ≈ V/6) Minimum flange (≈ V/2 + t)
0.8 mm 1.0 33% ≈4.8 mm 3.2 mm
1.2 mm 1.5 25% ≈7.2 mm 4.4 mm
1.6 mm 2.0 20% ≈9.6 mm 5.6 mm
2.0 mm 2.5 17% 12 mm 6.8 mm

Two bends in the same 0.8 mm S250GD+ZM310 sheet: R/t 1.0 on a 4.8 mm V-die cracks the coating, R/t 2.5 on a 12 mm V-die passes

The cost is visible in the last two columns: a larger radius needs a wider die, a wider die needs a longer flange, and a longer flange needs more material or a different part geometry. Springback also rises with R/t, so a wider die needs more angle correction. None of that is expensive next to a rejected lot, but it has to be decided at the drawing stage, not at the brake.

When the coating cracks, what actually fails

A coating crack is not a structural failure, and it is easy to dismiss as cosmetic. It is not, for three reasons:

  • It starts corrosion in the one place you cannot inspect. Underfilm corrosion propagates along the coating–steel interface, away from the crack, so the visible defect stays small while the affected area grows.
  • It discards the reason the coating was specified. Zn-Al-Mg and Zn-55%Al are chosen for cut-edge and scratch protection; a cracked bend is the same failure mode the coating exists to prevent.
  • It fails the qualification test, not the part. Salt spray (ISO 9227), adhesion after bending (ISO 2409 cross-cut on a bent coupon) and the T-bend are the tests a coated part is accepted on, and a cracked bend fails them before the product ever sees service.

The failure itself is usually a series of fine transverse cracks across the radius, sometimes only at the outer edge of the bend where the strain is highest, sometimes along the grain if the bend runs with the rolling direction. On prepainted sheet it appears as microcrazing and gloss change, then blistering as moisture reaches the interface.

The same limit in stamping geometry

Stamping does not change the strain criterion, but it changes where the strain lands, which is why a drawn part can fail at a radius that a simple press-brake bend would survive.

At the die entry. As the sheet is drawn over the die radius it is bent and unbent, so the die radius is a bend with an R/t of its own. A die radius below about 4t concentrates strain at the entry and is one of the most common causes of splitting in a drawn box; 6–8t is normal for mild steel, and 8–12t for dual-phase and high-strength grades.

At the punch nose. The punch radius forms the inside corner of the drawn feature, so the same R/t table applies to it. Bottom corner radii below about 1t are where splits begin; 2–3t is the practical design range, and vertical corner radii want at least 3t, larger again where the draw is deep.

At the flange and hem. A hem folds the sheet flat on itself, which is an R/t near 0.5 at the fold — far harsher than any brake bend. Hemming therefore depends on elongation and edge condition rather than on radius: about 20–25% total elongation is the usual floor, sheared edges may need deburring or a laser edge, and dual-phase steels typically need a pre-hem or a rope hem because they will not take a flat hem at all.

At a sheared edge. A cut edge is a stress raiser, and in high-strength and dual-phase steels the edge is often the initiation site rather than the radius. Hole expansion ratio is the relevant property — high for mild steel, falling to the 20–40% range for DP980 — and a laser or waterjet edge performs consistently better than a sheared one because the burr and the work-hardened layer are absent.

How to resolve a cracking bend

The options are ordered by cost, and the first three solve the S250GD+ZM310 case without changing the part’s function.

1. Increase the radius. Open the die, or specify a radius that needs a wider die. This costs flange length and material, and it is the only lever that changes the strain directly. It is almost always cheaper than a material change.

2. Bend across the grain. A bend whose axis is parallel to the rolling direction puts the strain along the grain structure and is markedly less forgiving on the marginal materials — heavy coatings, half-hard tempers, high-strength steel. On ZM310 the difference between orientations is the difference between passing and failing. Rotating the flat pattern at nesting costs material and nothing else; see how grain direction affects sheet metal forming.

3. Change the coating, not the steel. ZM310 is a heavy coating chosen for corrosion life. ZM200 or ZM120 at the same thickness carries roughly a third to a half of the coating mass and a proportionally thinner intermetallic network, and it bends cleanly at R/t = 1.5. If the environment allows it, plain zinc or electrogalvanised is more formable again. The trade is corrosion margin, and that is a decision to take against the actual exposure, not against habit.

4. Change the substrate grade. S250GD is a structural grade. Where the strength is not needed, DX51D+ZM or an HX-formability grade has more elongation in reserve at the same yield level and tolerates a tighter radius. Where the strength is needed, moving down the table to S220GD is often enough.

5. Split the operation. Two shallow bends in sequence, or a pre-bend followed by a final form, distribute the strain instead of concentrating it. Roll forming does this by design — a long bend is formed progressively by many small radii, which is why coated profiles that would crack on a press brake are routinely roll-formed. For a long, straight bend on a heavy coating, roll forming is often the correct process rather than a workaround.

6. Form first, coat afterwards. Post-painting removes the film from the bend strain and replaces it with an edge-coverage question, which is a solved problem: pretreatment plus spray or powder reaches the bend, and the coating is not asked to survive the press. It costs a process step and a masking operation, and it does not help the metallic coating underneath.

7. Soften, form, then restore. Where a hardened temper is the constraint rather than the coating — 301 half-hard, 6061-T6, Grade 5 titanium, work-hardened brass — form in the annealed condition and heat-treat afterwards. This is standard in aerospace and adds distortion control that a general fabrication shop is not set up for.

8. Repair, and do not rely on it. A zinc-rich touch-up on a fine coating crack is a legitimate site repair for a painted structure, and it is not a substitute for a bend that did not crack. If the acceptance criterion is a salt-spray test, touch-up will not pass it.

What to put on the drawing

Most cracking problems are specification problems. A drawing that names the material and the coating but leaves the radius to be inferred will be built with the tooling that is already in the machine.

Field What a fabricable drawing states
Material The full designation, including the coating: S250GD+ZM310 per EN 10346, not “galvanised steel”
Bend radius The inside radius as a dimension, and R/t where the material is thin enough for the ratio to govern
Bend direction “Bend lines across the rolling direction” for marginal materials; silence means nesting decides
Coating acceptance The test and the pass level — T-bend 2T, no crack to substrate at 10×, adhesion after bending
Edge condition Deburred, laser-cut or sheared, because the edge is a crack initiation site on high-strength grades
Flange A minimum formed height consistent with the die the radius implies, roughly V/2 + t
Springback An angle tolerance that reflects the material, typically ±0.5° to ±1°, not a blanket callout

The general form of these requirements is in the sheet metal drawing and DFM checklist, and the tooling side — die opening, punch tip and minimum flange — is covered in press brake tooling selection.

How the limit is verified

Because the limit is a cracking criterion, it is tested rather than calculated:

  • Bend or T-bend on a coupon from the actual coil — EN 13523-7 for prepainted sheet, ISO 7438 for the metal itself, at the specified radius and direction.
  • Adhesion after bending by cross-cut (ISO 2409) on the bent coupon, which catches the interface failures a visual check misses.
  • Formability screening by Erichsen cupping (ISO 1520) where a deep-drawn feature is involved.
  • Coating mass and thickness by XRF (ISO 3497) or gravimetric methods (ISO 1460), because the coating designation on the certificate is a minimum, not a measurement.
  • Salt spray (ISO 9227) on the formed part, which is the only test that shows whether a marginal crack has cost you the corrosion life you paid for.

A formed coupon costs a few minutes and a scrap blank. It is the cheapest step in the whole chain, and the one most often skipped.

Summary

R/t is the controlling variable in bending and stamping: at R/t = 1.0 the outside of the sheet is stretched by roughly a third, and no coating of 20 µm of intermetallic-containing zinc alloy can follow that. Mild steel at 0.5–1.0t, stainless at 1.0–1.5t, HSLA at 2–3t, aluminium 6061-T6 at 4–6t are the substrate limits; heavy zinc-magnesium, aluminium-zinc and prepainted surfaces impose a stricter coating limit of 1.5–2.5t before the steel itself is anywhere near failure. Design to the ideal rather than the limit, remember that in air bending the die opening rather than the drawing sets the radius, and test a coupon from the coil that will actually be pressed.


Related reading: minimum bend radius by material, press brake tooling selection, how grain direction affects sheet metal forming, and SGCC vs SECC vs SPCC.

Send the drawing with the material and coating designation, the bend radius and the corrosion requirement, and the formable radius, the die opening and the flange limit can be confirmed for the actual gauge. Metal bending services and sheet metal stamping both run a formed coupon before the first production order.

Request a Free Quote

Send the project details below for drawing review and quotation planning.

By submitting you agree to our Privacy Policy.

We respect your privacy. Your information is secure and will never be shared.