Sourcing to US Standards: ASTM Grades, G90 Coatings and Mill Test Reports

Fabex Engineering Team September 30, 2026
Sourcing to US Standards: ASTM Grades, G90 Coatings and Mill Test Reports — Powder coated sheet metal parts

Sourcing to US Standards: ASTM Grades, G90 Coatings and Mill Test Reports

US drawings are precise about material and imprecise about one thing that matters most to a supplier: thickness. A drawing that says “16 ga galvanized, G90” contains a coating class a Chinese mill can match exactly and a thickness expressed in a system nobody outside North America uses.

Part 1 covered the substitution decision; this is the US case. The good news is that ASTM’s material families have close, well-understood Chinese equivalents. The trap is the units.

Standing caution. Cross-references are procurement directions, not certifications. Confirm each against the mill certificate and your engineer’s approval.

The ASTM standards behind most US sheet metal

Standard Covers Typical designations
A1008 cold-rolled carbon steel sheet, commercial and drawing quality CS Type B, FS, DS, DDS, EDDS; HSLA grades
A1011 hot-rolled carbon, structural and HSLA sheet and strip CS, SS Grade 36/40/50, HSLA
A653 hot-dip zinc-coated (galvanized) sheet G40, G60, G90, G115, with CS/FS/DS types
A792 55% aluminium-zinc coated sheet AZ50, AZ150
A240 stainless steel sheet and plate 304, 304L, 316, 316L
A36 / A572 structural carbon and HSLA steel A36, A572 Grade 50
A924 general requirements for metallic-coated sheet the testing rules behind A653/A792

A1008 versus A1011 is the distinction buyers most often skip. A1008 is cold-rolled: better surface, tighter thickness, better formability. A1011 is hot-rolled: cheaper, thicker scale, coarser tolerances. A part designed in cold-rolled and quoted in hot-rolled will be a different part — and a supplier may quote either if the drawing only says “sheet steel”.

CS Type B is the commercial-quality default in A1008. It is the closest US relative of DC01 (EN) and SPCC (JIS), which is why the substitution in China is usually straightforward.

The G90 conversion — and why it is the number that matters

A653 coating classes are stated in ounces per square foot, total on both surfaces. Converted:

A653 class oz/ft² g/m² total Closest metric class
G40 0.40 ~122 Z120-ish
G60 0.60 ~183 Z180
G90 0.90 ~275 Z275
G115 1.15 ~351 Z350
A792 AZ150 0.50 150 (Al-Zn) AZ150

G90 and Z275 describe the same order of coating mass. That single line resolves most US-to-China galvanizing conversations. Two cautions:

  • Total versus per side. A mill quoting “Z120 double-sided” is not offering a G90. Ask for the mass and the basis in writing.
  • Alloy, not just mass. A792’s aluminium-zinc is a different coating from A653’s zinc at the same mass. AZ150 is not interchangeable with G90 for the same environment, even though the numbers are close.

Gauge: the specification that causes scrap

US drawings frequently state thickness as a gauge number. Gauge is not a dimension — it is a table lookup that differs by material and by convention. A supplier working in millimetres has to convert, and a rounding error of 0.05 mm is enough to change a bend result or a fastener fit.

Gauge Decimal (in) Millimetres Note
24 ga 0.0239 0.61 light cover panels
22 ga 0.0299 0.76
20 ga 0.0359 0.91 common enclosure wall
18 ga 0.0478 1.21
16 ga 0.0598 1.52 bracket and chassis work
14 ga 0.0747 1.90
12 ga 0.1046 2.66 heavier structure
11 ga 0.1196 3.04

The practical instruction: put the decimal and the millimetre on the drawing, not the gauge alone. It costs one sentence and removes an entire class of remake. Also state the thickness tolerance — A1008 and A1011 have different tolerance ranges, and “16 ga” does not pin one.

Structural: A36, A572 Gr 50 and the strength question

  • A36 is the historical US structural default: 36 ksi minimum yield, roughly 250 MPa.
  • A572 Grade 50 is the workhorse HSLA structural grade: 50 ksi minimum yield, roughly 345 MPa.

In Chinese-mill terms, A572 Gr 50 sits in the Q355 / S355 family, and A36 sits around Q235/Q355 depending on thickness. As with the European and Australian cases, the strength is the easy part; what needs confirming is whether the design depends on anything else — impact toughness, weldability limits, or a certified structural execution requirement.

If the part is genuinely structural and welded to a US code, the welding procedure and qualification are part of the specification. That is a fabricator capability, not a steel purchase. Say whether the part is structural; it changes both the supplier you need and the paperwork.

Certificate language: MTR and what it does not prove

US buyers ask for an MTR — mill test report. In Chinese supply, an MTR is usually issued in the EN 10204 formats, most often 3.1, which is the strongest of the routine documents: named test results for the delivery, endorsed by the mill’s independent inspection representative.

What an MTR proves: the material in the delivery matches the chemistry and mechanical properties claimed.

What it does not prove: that the coating mass is what the drawing asked for (that needs coating testing, which A924 describes), that the part geometry is right, that the weld is sound, or that the fabricator’s process is controlled. Buyers sometimes treat an MTR as a general quality certificate. It is a material statement with a narrow scope — useful, and not a substitute for first-article inspection.

If the end customer needs third-party verification, an independent laboratory test of the delivered material (SGS or comparable) can be arranged per order. That is a different product from an MTR and is priced separately.

The sensible substitutions for a US drawing

Specified Practical Chinese equivalent What to confirm
A1008 CS Type B SPCC (JIS) / DC01 (EN) formability grade if the part is drawn
A1011 CS SPHC / Q235 hot-rolled thickness tolerance — hot-rolled ranges are wider
A653 G90 SGCC at 275 g/m² total coating mass and basis; not A792
A653 G115 SGCC at ~350 g/m² total availability at low volume
A792 AZ150 AZ150 aluminium-zinc alloy identification, not just the mass
A240 304 / 316L SUS304 / SUS316L nickel and molybdenum, by certificate
A572 Gr 50 Q355B / S355 impact requirements if the design relies on them
A36 Q235 / Q355 thickness-dependent yield; check the certificate

What to put on the drawing for a US job

  • Standard, grade and type — “A653 G90, CS Type B, 0.91 mm” beats “16 ga galv”.
  • Decimal thickness and tolerance class, alongside any gauge reference.
  • Coating mass on a stated basis, and whether cut edges need protection.
  • Whether the part is structural, and which welding standard applies if so.
  • The MTR requirement, and whether third-party testing is needed on top.
  • Confirmation of gauge convention if a gauge number survives — sheet steel gauges are not the same as stainless or aluminium gauges.

The summary

The US system is the most mechanically explicit of the three and the easiest to substitute safely if the units are converted properly. G90 maps cleanly onto Z275; A1008 CS Type B maps onto SPCC; A572 Gr 50 maps onto the Q355 family. The recurring risk is not metallurgy, it is gauge arithmetic and the assumption that an MTR certifies more than the material.

That closes the series. The Australian and European parts cover the same decision under different naming and different certificate languages. If you want a US drawing reviewed for what is actually buyable at your quantity — including an explicit note on any gauge conversion — send it over with the end use stated.

Request a Free Quote

Send the project details below for drawing review and quotation planning.

By submitting you agree to our Privacy Policy.

We respect your privacy. Your information is secure and will never be shared.